A chunk of concrete on the balcony floor. A rust-colored streak running down from the edge of a slab. A column corner that has popped off and shows a dark bar underneath. Those are the classic signs of spalling, and they call for concrete spalling repair planned by an engineer. A hairline crack running from the corner of a bedroom window is a different problem with a different fix. Knowing which one you are looking at decides who you call first.
What concrete spalling is
Columns, beams, balcony slabs and many walls on South Florida buildings are reinforced concrete: concrete with steel bars (rebar) cast inside. Concrete normally protects that steel. Penn State's civil engineering course notes explain that the steel "is usually protected from corrosion due to the high pH (~ 12.5)" of the cement's hydration products. Chlorides, the salt in sea spray and salty water, break through that protection and let the steel start to rust.
Rust takes up more room than the steel it came from. The same notes put it this way: "The rust produced will have significantly higher volume than the original steel," and that growth puts internal stress on the concrete around it. "The corroded steel essentially pushes outward on the concrete, causing it to delaminate, crack and eventually spall."
So the piece that falls off is the last stage of a process that started inside the concrete. By the time you see spalling, the steel has usually been corroding for a while, and the area around the visible damage may already be cracked or separated below the surface.
Why salt air makes it worse here
FEMA's coastal construction guidance says "Metal corrosion is most pronounced on coastal homes (within 3,000 feet of the ocean)," and adds that reinforcing steel "should be protected from corrosion by sound materials." Plenty of condo towers in Miami Beach, Sunny Isles, Hollywood, Fort Lauderdale and Pompano Beach sit well inside that distance.
The rules reflect it. Florida Statute 553.899 lets a local building official require the first milestone inspection at 25 years instead of 30 when local conditions such as "proximity to salt water" call for it, and Miami-Dade's 2023 recertification guidance sets 25 years for condos and co-ops three stories or taller within 3 miles of the coastline. Our milestone inspection guide covers those programs in detail.
What investigators found at Champlain Towers South
The partial collapse of Champlain Towers South in Surfside on June 24, 2021 took 98 lives. The National Institute of Standards and Technology (NIST) released its technical findings in June 2026. NIST says the collapse began in early June 2021, when two connections between garage columns and the pool deck failed, and it lists "long-term degradation from corrosion" among the factors that reduced the building's margin against failure.
In its public presentation of those findings, NIST said "corrosion of reinforcing steel was evident more than 25 years before the collapse" and that structural repairs and waterproofing were done in 1996 and 1997. After those repairs, "There was continued leakage and rust staining," and in some locations "the concentration of chloride was high enough to sustain corrosion of the reinforcing steel." Corrosion was heavier under planters and in spots with "high exposure to chloride-laden water," and NIST said degradation was made worse by "porous concrete, concrete cracks that leaked, and ineffective waterproofing."
That collapse had many causes, including design and construction problems that a homeowner or board could not see. The part that applies to everyday buildings is simpler: leaks, rust stains and corroding steel in concrete are engineering matters, and covering them up does not stop the corrosion.
How spalling differs from a stucco crack
Stucco is a cement plaster layer over the block or concrete. The residential code's minimums run from 1/2 inch on masonry to 7/8 inch over wire lath. Spalling happens in the concrete itself. Some practical differences:
- Location. Stucco cracks show up most often at the corners of doors, windows and other openings, according to a Sika technical bulletin. Spalling shows up where steel sits close to the surface of concrete: slab edges, the undersides of balconies, column corners and beams.
- Color. A stucco crack is usually the color of the wall, maybe with a dirt line. Spalling often comes with brown or orange rust staining, and sometimes you can see the bar itself.
- What comes off. A stucco crack stays a line. Spalling drops pieces of concrete, sometimes with a rough, rusty face on the back.
- Width and movement. NAHB engineering guidance treats cracks up to 1/8 inch wide as negligible to slight, and says cracks are more of a structural concern when they come with signs like doors and windows that stop working, or when one side of the crack sits higher than the other.
The two can overlap. Stucco applied over a concrete column or beam will crack when the concrete behind it starts to spall, so a stucco crack with a rust stain bleeding through it should be treated as a possible concrete problem until an engineer says otherwise.
Where it shows up on South Florida buildings
- Balcony slab edges and the underside of the balcony above you
- Columns and beams, especially at corners. Miami-Dade's recertification list names "spalling" for columns, beams and slabs
- Garage ceilings and pool decks, where water can sit on or seep through the slab
- Planters built on slabs, which NIST found were among the worst spots for corrosion at Champlain Towers South
- Elevated decks and walkways. Broward's BORA Policy 05-05 inspection includes "elevated decks, balconies, docks, and seawalls" attached to or supporting a structure
Who repairs spalling
Spalling is structural work. Florida Statute 489.117 lets anyone do "plastering" and "stuccoing" without a state license, but repair of the concrete, block, beams or steel behind the stucco is a separate scope that may need an engineer and a licensed contractor. The permit rules follow the same line. The state's new permit exemption for small single-family jobs (HB 803, in effect since July 1, 2026) does not cover structural work, and Miramar's stucco permit package requires plans signed and sealed by a professional engineer if any structural repair is included.
On a condo or commercial building, the engineer's milestone or recertification report usually sets the repair scope. A local stucco contractor fits in after the concrete is repaired: rebuilding the stucco over patched columns and slab edges, matching the texture, and fixing the ordinary stucco cracks elsewhere on the building. See condo and commercial stucco restoration for how that part of the job works.
What to do if you see it
- Keep people and cars out from under any area where concrete is falling.
- Take photos: a wide shot that shows where on the building it is, and a close-up with something for scale, like a coin or a tape measure.
- In a condo, tell the manager or the board in writing so it reaches their engineer. On a house, call a structural engineer.
- If it turns out to be stucco cracking only, the fix is ordinary stucco crack repair.
Not sure which one you have? Send photos through the contact page or call (954) 371-2314. If it is stucco, a local stucco contractor quotes it. If it looks like concrete, you will be told it needs an engineer first. Hablamos español.
Questions
Is concrete spalling dangerous?
It can be. Spalling means the steel inside the concrete is rusting, and loose pieces can fall. NIST's Champlain Towers South findings note that moderate corrosion can significantly reduce the capacity of connections. Keep people clear of the area and have an engineer look at it.
Can a stucco contractor fix concrete spalling?
The concrete and steel repair is structural work that may need an engineer and a licensed contractor, and the state's small-job permit exemption does not cover structural work. Florida law lets anyone do stuccoing and plastering, so a stucco contractor typically handles the stucco and finish work once the concrete is repaired.
How can I tell spalling from a stucco crack?
Look for rust. Spalling usually comes with brown or orange staining, missing chunks of concrete, or visible steel, often at slab edges, balconies and column corners. A stucco crack is usually a thin line, most often at the corners of windows and doors.
Why is spalling more common near the beach?
Salt. Chlorides from sea spray break down the protection that concrete gives its steel, and the rusting steel expands and cracks the concrete. FEMA guidance says metal corrosion is most pronounced within 3,000 feet of the ocean.